Resin glass flake cement (coating)
> Glass flake primer
) Take the pre-prepared appropriate amount of primer, then add the appropriate proportion of matching curing agent and stir. Use evenly. Use a brush or roller to apply the paint, and the amount should be about 1 square meter per road. Apply the first coat of primer to the prepared surface to be lined. And apply a second coat of primer after the first coat of primer. The directions for applying primers should be perpendicular to each other.
) During the construction of steel structure foundation, during the process of mixing primer and rubber, quartz powder (about mesh) with a weight ratio of % resin should be added. Only after mixing evenly can the construction achieve better results. Interface bonding effect.
) During concrete foundation construction, if the viscosity is slightly high or in a low-temperature construction environment, in order to increase the bonding between the coating and the base layer, % solvent can be appropriately added for dilution. The solvent is preferably styrene. , the primer can be applied all over.
Glass flake cement mid-coat
) The mid-coat resin should match the base coating resin. The viscosity of glass flake coating is generally to The thickness of each layer is about 100 Å, which varies with different construction methods. Construction can be done by roller brushing or spraying, and high-pressure airless spraying should be used for spraying.
) When preparing glass flake paint, a stirrer with a higher rotation speed should be used. Add an appropriate proportion of matching curing agent and stir for more than 10 minutes. The flake glue paint stirred at one time should be used up within the time limit. , and the initial setting time should be controlled at around .
) After the previous layer is dry, the next layer of construction can be carried out. The dosage is about / square meter. The painting direction of the paint should be consistent, and the painting direction between the two layers should be vertical. The coating should be uniform, no missed coating is allowed, no sagging bubbles, pinholes and debris (brush bristles, sand particles, etc.), and other defects are not allowed.
) Apply a layer of chopped strand felt to the uneven surface and structural corners for local reinforcement. Use a roller to apply a layer of paint and then add a layer of glass felt. After soaking, use a roller impregnated with the paint to brush. Remove the air bubbles. Then carry out construction according to the above construction requirements.
Plexiglas flake coating topcoat
Since corrosive media directly contacts the outer surface of the coating, the topcoat resin must have excellent corrosion resistance and minimize the use of fillers. Dosage. At the same time, the topcoat also plays a role in beautifying the appearance of the coating and increasing its impermeability. When preparing the coating, add an appropriate proportion of the matching curing agent and stir for more than 10 minutes before construction. Generally, the dosage is about 100 square meters per lane. The last coating should contain styrene paraffin liquid.
<
<
<
<
<
<
<